(1) Influence of Water Quality
If the water used in the tank contains severe rust or has high levels of calcium and magnesium ions, it will affect the stability of the surface treatment solution. When preparing the tank solution, a water softener can be added in advance to mitigate the impact of water quality on the surface treatment solution.
(2) Usage Time
Typically, surface treatment agents use colloidal titanium salts, which possess colloidal activity. When the usage time is long or the solution contains many impurity ions, the colloidal activity will be lost. At this point, the colloid's stable state is destroyed, the tank solution precipitates and layers, forming a flocculent appearance. At this time, the tank solution must be replaced.
Phosphating Process
The phosphating process is a chemical and electrochemical reaction that forms a phosphate chemical conversion film, and the formed chemical conversion film is called a phosphating process film. In bus painting, the commonly used solution is low-temperature zinc-based phosphating solution. The main purpose of the phosphating process is to provide protection for the base aluminum material and to a certain extent prevent the aluminum from being corroded; it is used as a primer before painting to improve the adhesion and corrosion resistance of the paint film. The phosphating process is a very important part of the entire pretreatment process. Its reaction mechanism is complex and there are many influencing factors; therefore, the process control of phosphating bath solution is much more complicated compared to other bath solutions.
(1) Acid Ratio
Increasing the acid ratio can accelerate the reaction speed of the phosphating process, making the phosphating process film thin and delicate. However, if the acid ratio is too high, the film layer will be too thin, easily causing the phosphated workpiece to collect residue; if the acid ratio is too low, the phosphating process reaction speed will be slow, the phosphating crystals will be coarse and porous, corrosion resistance will be low, and the phosphated workpiece will easily develop yellow rust. Generally speaking, the required acid ratio varies depending on the phosphating solution system or formula.
(2) Temperature
Properly increasing the bath temperature can accelerate film formation, but if the temperature is too high, it will affect changes in the acid ratio, thereby affecting the stability of the bath. At the same time, the film nuclei become coarse, and the amount of sludge from the bath increases.
(3) Amount of Sediment
As the phosphating process continues, the amount of sediment in the tank liquid will gradually increase. Excessive sediment can affect the interfacial reaction on the surface of the workpiece, causing the phosphating film to be uneven, with severe ash attachment, or even fail to form a film. Therefore, the tank liquid must be timely replaced according to the amount of workpieces being processed and the duration of use to remove the sediment and sludge.
(4) Nitrite NO-2
NO-2 can accelerate the phosphating process, improving the film's density and corrosion resistance. If the content is too high, the film may develop white spots or color iridescence; if too low, the film formation rate is slow, and the phosphating film is prone to yellow rust.
(5) Sulfate Ion SO4²⁻
If the concentration of the pickling solution is too high or the rinsing is not well controlled, it can easily lead to an increase in sulfate ions in the phosphating process solution. Excessive sulfate ions will slow down the reaction rate of the phosphating process, making the phosphating film grains coarse and porous, causing severe gray deposits, and reducing the corrosion resistance of the phosphating film.
(6) Ferrous Ion Fe²⁺
When the amount of ferrous ions in the phosphating solution is too high, it can reduce the corrosion resistance of room temperature phosphating films; cause medium temperature phosphating film grains to become coarse, surfaces to turn whitish-gray, and reduce corrosion resistance; and increase sediment formation in high temperature phosphating solutions, making the solution turbid while also increasing the free acidity.