Main Cause Analysis:
① The extrusion temperature of the aluminum profile is too low, and the extrusion speed is too slow. The profile does not reach the solution treatment temperature at the outlet of the extruder, so solution strengthening cannot take effect;
② There are few fans at the profile outlet and insufficient air volume, resulting in slow cooling speed. This prevents the profile from dropping below 200°C in the shortest time, causing coarse Mg2Si to precipitate prematurely, thereby reducing the solution phase and affecting the mechanical properties of the profile after heat treatment;
③ The composition of the ingot is unqualified, with Mg and Si content in the ingot not meeting standard requirements;
④ The ingot has not undergone homogenization treatment, so the Mg2Si phase precipitated in the ingot structure cannot be re-dissolved during the relatively short extrusion time, resulting in insufficient solution and affecting product performance;
⑤ Improper aging process, poor hot air circulation, or incorrect thermocouple installation location, leading to insufficient aging or over-aging.
Solution:
① Reasonably control the extrusion temperature and extrusion speed, keeping the profile temperature at the exit of the extruder above the minimum solution temperature;
② Enhance air cooling conditions; factories with the capability can install atomization cooling devices to meet the minimum cooling gradient requirements of 6063 alloy;
③ Strengthen the quality management of ingots;
④ Perform homogenization treatment on the ingots;
⑤ Reasonably determine the aging process, correctly install thermocouples, and properly place profiles to ensure smooth hot air circulation. Geometric dimension deviation.