Aug 21, 2025 Leave a message

Melt casting production safety operation regulations-1

Melt casting production safety operation regulations

1. Purpose Make normative regulations on the operation technology of each process in the process of casting production, and guide the operation behavior of on-site operators to ensure the quality and safe production of cast aluminum rods.

 

2. Scope of application
This regulation applies to the safety and operation guidance of the production process of aluminum alloy casting rods in the melting and casting workshop of the aluminum factory.

3. Enforcement and supervision

2.1 The workshop director is responsible for guiding and supervising the workshop employees to operate in accordance with the provisions of this regulation.

2.2 Employees in all positions should strictly follow the provisions of this regulation to carry out production operations.

 

4. Smelting operation procedures
4.1 Oven
4.1.1 Newly built or overhauled melting furnaces must go through strict ovens before they can be put into use.
4.1.2 Before the melting furnace that has been shut down for a long time (more than one month), press the 2/3 furnace door to heat up to 150 °C for 8 hours, close the furnace door to heat up to 700 °C for 10 hours, and then start feeding and smelting.

4.1.3 For furnaces with a shutdown time of more than 24 hours to less than one month, before the furnace is opened, it needs to be heated to 250-300 °C for 3 hours for drying, and then the material can be added to start melting.

4.2 Wash the furnace
4.2.1 The furnace must be washed when the furnace is new, overhauled, or intermediate, and when the smelting alloy grade is changed (with large differences), or when the 7 series alloy is smelted and then transferred to other alloys.
4.2.2 The furnace can be washed with the return furnace material of the building profile, and the amount of washing material shall not be less than 20% of the furnace capacity.
4.2.3 When the melt heating temperature is 800~850°C, stir thoroughly three times, and the interval between each stirring is 20 minutes.

4.2.4 Whether the melting furnace needs to be washed after the long-term shutdown is determined by the director of the casting workshop according to the specific situation.

4.2.5 When washing the furnace charge and casting, the aluminum liquid in the furnace must be completely discharged.

4.3 Clearing furnace

4.3.1 After each melting furnace has been continuously produced for 20~30 melts (or when the amount of furnace content is seriously insufficient), the furnace should be thoroughly cleared before stopping.

4.3.2 When cleaning the furnace, the furnace temperature is required to rise to 800°C~900°C, sprinkle with slag breaker, and use a furnace cleaning shovel to remove and clean the slag on the furnace wall and corner.

4.3.3 When removing the slag after each melting, the slag and other dirt on the surface of the melt must be carefully and thoroughly removed to ensure the purity of the furnace body and the capacity of the furnace.
4.4 Furnace installation

4.4.1 Furnace loading sequence: small piece - tube, type, bar - plate - aluminum ingot - large scrap - intermediate alloy.

4.4.2 The feeding material must ensure that the alloy grade is accurate. The ingredients are clear, clean and dry, and should not be mixed with other metals and debris.

4.4.3 The furnace charge should be added as much as possible, if it cannot be loaded at one time, it should not be stacked too high at one time, and a certain space should be maintained in the furnace; When the first loaded furnace charge is leveled, the second charge should be loaded according to the furnace charge.

4.4.4 When there is aluminum liquid in the furnace for secondary feeding, generally after the aluminum ingots begin to melt, the waste should be added by immersion to prevent the aluminum liquid from splashing and burning people.

4.4.5 Intermediate alloys such as aluminum and silicon are added with the last batch of charge.

4.4.6 After slag removal, when the melt temperature is not lower than the lower limit of the melting temperature, press the magnesium ingots into the aluminum liquid with a bell jar and add them, and sprinkle them with No. 3 flux to cover.

4.4.7 Pay close attention to the aluminum water liquid level after the furnace is installed to prevent the overflow of aluminum water from causing safety accidents.

 

4.5 Open the furnace for melting

4.5.1 Before starting the furnace, it should be operated under no load, and the motor and fan should be checked without abnormal sound and normal operation. and clean up equipment and workplace obstacles.

4.5.2 Check that the furnace door chain is firm and reliable, and the furnace door should be opened and closed flexibly.

4.5.3 Check that the exhaust and exhaust system and permanent magnet mixing system equipment are normal.

4.5.4 Check that the furnace wall, furnace bottom, and furnace wall should be intact and whether there is any loosening or falling off.

4.5.5 Check that there should be no foreign debris in the furnace.

4.5.6 The melting process is strictly operated in accordance with the "Safety Regulations for the Use of Natural Gas", confirm that the furnace door and flue gate are open before ignition, and open the fan after starting the ignition. If the first ignition fails, the gas in the furnace must be blown out before it can be ignited again, otherwise it will cause a gas explosion accident.

4.5.7 Adjust the musket damper and pressure to make the flame bright, no black smoke, and close the furnace door only after the burner is working normally.

4.5.8 When the charge softens and collapses, small pieces of aluminum waste should be added in time and slowly pressed into the aluminum liquid to reduce oxidative burning loss.

4.5.9 During the melting process, it must be stirred manually or with a permanent magnet stirrer 3~4 times to make the temperature of the melt even, prevent local overheating of the aluminum liquid, and shorten the melting time.

4.5.10 In principle, the temperature of the aluminum liquid shall not exceed 760 °C in the whole melting process, and the specific parameters are according to the "Technical Regulations for Melting and Casting Process", and the melt temperature is too high and the air absorption is serious.

4.5.11 Inspect the furnace body and aluminum outlet, and if aluminum leakage is found, it should be plugged and repaired in time.

4.5.12 In accordance with the content stipulated in the melting process regulations, the process parameters are set on the touch screen of the control cabinet, and the relevant melting safety operation procedures are implemented.

4.5.13 During the implementation process, according to the actual needs, the hot air circulation and the smoke collection and treatment system can be opened and closed in a timely manner.

4.5.14 According to the process requirements, a series of process operations such as refining, degassing, stirring, and slag removal of the aluminum liquid in the furnace are completed and ready for casting.


4.6 Pick up slag

4.6.1 The melt temperature should rise to 730~750°C before slag removal, which is convenient for the separation of aluminum slag during slag removal and the separation of aluminum slag in subsequent ash frying operation.

4.6.2 When the slag is picked up to the furnace mouth, stop for a while and then remove it from the furnace to reduce the aluminum liquid brought out with the slag.

4.6.3 The slag rake should be kept stable when peeling slag, and from far to near, do not add the floating standard to the aluminum liquid, and try to completely remove the scum.

4.7 Stirring

4.7.1 Start stirring 5~10 minutes after adding magnesium.

4.7.2 According to the actual needs of production, adjust the permanent magnet mixer equipment to manual mode or automatic mode, and reasonably design the operating parameters.

4.7.3 The melt should not be stirred up too much wave during stirring to prevent surface oxides from being caught in the melt and increasing the damage.

4.7.4 Do a good job in daily equipment maintenance for the permanent magnet mixer according to the equipment maintenance requirements.

4.8 Sampling

4.8.1 After the melt is fully stirred, the sample should be taken immediately, and the pre-furnace analysis should be carried out, and the feed or dilution material should be determined according to the analysis results.

4.8.2 The sampling temperature shall not be lower than 710°C.

4.8.3 The sampling position should be controlled at about one-half of the melt depth in the center of the furnace.

4.8.4 Before sampling, the sampling spoon should be clean and preheated.

4.9 Adjust the ingredients

4.9.1 Replenish (or dilute) according to the results of pre-furnace composition analysis and the "Alloy Chemical Composition Internal Control Standard". The principle of feeding is to ensure that the proportion of each alloying element and the composition of the magazine element are within the allowable range of the specified internal control standards.

4.9.2 Stir well after feeding.

4.10 Refinement

4.10.1 Nitrogen for aluminum melt refining must be dried.

4.10.2 The solvent must have moisture-proof packaging and should not be opened before use to prevent water absorption.

4.10.3 When refining, the air source is opened first, and then the refining tube is inserted into the melt.

4.10.4 Refining with nitrogen spraying powder should ensure the refining time, the refining pipe should move slowly at the bottom of the melt pool, leaving no dead ends, and pay attention not to touch the refining tube to the bottom and wall of the furnace to prevent blockage of the refining pipe. After refining, the scum on the surface of the melt should be cleaned and covered with melt as required.

4.10.5 After refining, let it rest, adjust the temperature, and prepare for casting. The rest time is 20~30 minutes.