
The reasons for the yellowing phenomenon of electrophoretic aluminum profiles are summarized as follows: electrophoretic paint itself; Poor oxidative conductivity; not washed thoroughly before electrophoresis; over-curing; Oxidation tank fluid contaminated with nitric acid:
1. Yellowing phenomenon caused by poor conductivity of aluminum profiles during oxidation
If the aluminum profile is in poor contact with the conductive rod, the resistance at the contact will increase greatly, the end of the profile will heat up, the oxide film will be generated too quickly and accompanied by cauterization, and even the powdering of the oxide film will occur. At this time, the oxide film is a little cloudy, the color turns yellow, and if electrophoresis production is carried out, there will be a very obvious yellowing phenomenon. This yellowing phenomenon is usually only a few in a row, and basically appears at the end of the profile. Therefore, it is important to take measures to ensure that the aluminum profile has good contact with the conductive rod.
2. Yellowing phenomenon caused by incomplete washing before electrophoresis
The oxide film is honeycomb-shaped, and its porous structure determines that sulfuric acid will remain in the pores of the oxide film. As we all know, if the profile used for electrophoresis is not washed thoroughly, it is likely to yellow. For this yellowing phenomenon, it is generally believed that the acid roots in the oxide film pores react with the electrophoretic paint to cause the yellowing of the electrophoretic paint film, in fact, this yellowing is not the yellowing of the paint film, but the yellowing of the oxide film. If there is more sulfate remaining in the oxide film pores, the oxide film will react with the sulfate at high temperatures, so that the clear and transparent oxide film becomes cloudy and the transparency decreases; At the same time, coupled with the high transparency of the electrophoretic paint film and the high reflectivity of light, this defect is further amplified, forming the so-called yellowing. Therefore, several washes before electrophoresis are very critical, not only to ensure the quality of the washing water, but also to ensure the washing temperature and washing time.
3. The yellowing phenomenon caused by the contamination of the oxidation tank liquid with nitric acid
In order to achieve a better ash removal effect, it is understandable to add a certain proportion of nitric acid in the neutralization tank, but if the water washing control is not good after neutralization, nitric acid will be brought to the oxidation tank, and when the nitrate in the oxidation tank reaches a certain concentration, it will have a certain impact on oxidation, and even cause yellowing of the electrophoretic profile. During the oxidation process, the nitrate entering the pores of the oxide film will etch the oxide film, corrode the barrier layer of the oxide film, make the pores of the oxide film deeper, and then change the structure of the pores of the membrane. This corrosion has two effects on the oxide film: 1. The barrier layer of the oxide film becomes thinner, and the tightness of the bond with the aluminum matrix becomes poorer, which in turn causes the adhesion of the oxide film to decrease. 2. Under normal washing conditions, it is difficult to eradicate the sulfuric acid in the membrane pores. Electrophoretic profiles produced under these conditions are also subject to yellowing. How can we avoid this yellowing? Add neutralizer to the pure water tank before scalding the tank, adjust the PH value to 8~9.5, wash with water for 2~3 minutes, neutralize the sulfate in the oxide film pores with amine roots, and then carry out electrophoresis production, and there will be no yellowing.
4. Yellowing phenomenon caused by excessive curing
At present, the electrophoretic paints used in the market are basically baked and cured under the condition of 180°CX30min. Under normal conditions, the paint film basically does not turn yellow. However, the temperature of some manufacturers of curing furnaces is very uneven, and the local temperature difference is even more than 30°C; The temperature control system of some manufacturers is poor, the actual temperature is too different from the displayed temperature, and the yellowing phenomenon of poor quality electrophoretic paint is very obvious under this condition, even like coloring. Good quality electrophoretic paints have a strong tolerance for such extreme conditions, and some electrophoretic paints will not turn yellow even if baked at 230°C. In order to prevent yellowing, the uniformity of the furnace temperature, the sensitivity of the temperature control system are necessary, and the use of good quality electrophoretic paint is also necessary.
5. The yellowing phenomenon caused by the electrophoretic paint itself
Anodizing electrophoretic paints are mainly composed of acrylic resins and amine resins. During the baking process of the electrophoretic profile, the resin undergoes a cross-linking reaction to produce a flat, transparent coating film. However, some electrophoretic paint manufacturers use poor quality chemical raw materials due to the immaturity of the production process, or in order to reduce costs, resulting in a relatively narrow curing range. The baking is slightly insufficient, and the hardness of the paint film is not enough; If the baking is slightly overdone, the paint film will turn yellow, which will bring certain difficulties to production management. Therefore, it is recommended that you choose a paint supplier with stable product quality and a certain reputation.




